KTI is a most leading brand in the Plywood Market in Delhi NCR. We are working with a proficient team of trained and professional engineers who are working with us. KTI has now become a dream of today’s time to design the interiors and modify the decors with the most beautiful furniture and designs. KTI plywood is made with the help of thin layers of wood veneers glued together with the best quality adhesive to make them strong and more durable. We have MR Grade and BWR Grade Plywood
Technical Specification (IS – 303 : 1989) | |||
Serial No. | Test | BIS Requirement | Observed Value |
1. | (Dimension) Length | Length +6 / -0 (mm) | Length +2 mm |
Width | Width +3 / -0 (mm) | Width +1 mm | |
Thickness | up to 5 mm +10%/-10% 6 mm & Above +5%/-5% | 3.12% 3.25% | |
Squareness | 0.20% | 0.11% | |
2. | Moisture Content | 5-15% | 6.70% |
3. | Glue Adhesion Water Resistance Test | ||
3 Cycles at 60 +2/-2 0C for 3 hours immersion in water and dried for 3 Cycles of 8 hours at 65 +2/-2 0C in Alternate wet and dry Process | Adhesion of Plies should be min. Pass Standard | Excellent | |
4. | Static Bending Strength | ||
MOR Along the Grain | Avg. – 30 N / mm2 Ind. – 27 N / mm2 | Avg. 34.20 N / mm2 Ind. 31.41 N / mm2 | |
MOR Across the Grain | Avg. – 15 N / mm2 Ind. – 13 N / mm2 | Avg. 21.60 N / mm2 Ind. 19.63 N / mm2 | |
MOE Along the Grain | Avg. – 4000 N / mm2 Ind. – 3600 N / mm2 | Avg. 4563.14 N/mm2 Ind. 4285.93 N/mm2 | |
MOE Across the Grain | Avg. – 2000 N / mm2 Ind. – 1800 N / mm2 | Avg. 2452.55 N/mm2 Ind. 2288.16 N/mm2 | |
5. | MyCological Test | Min. Pass Standard | Pass Standard |
6. | Workmanship And Finish | Should be Conforming to The Requirements of Cl. 9.1 & 9.2 of IS – 303 : 1989 | Conforming |
Technical Specification (IS – 303 : 1989) | |||
Serial No. | Test | BIS Requirement | Observed Value |
1. | (Dimension) Length | Length +6 / -0 (mm) | Length +1 mm |
Width | Width +3 / -0 (mm) | Width +1 mm | |
Thickness | up to 5 mm +10%/-10% 6 mm & Above +5%/-5% | 3.21% 2.89% | |
Squareness | 0.20% | 0.13% | |
Edge Straightness | 0.20% | 0.09% | |
2. | Moisture Content | 5-15% | 7.20% |
3. | Glue Adhesion Water Resistance Test | ||
3 Cycles at 100 +2/-2 0C for 8 hours Boiling in water and dried for 3 Cycles of 16 hours at 65 +2/-2 0C in Alternate wet and dry Process | Adhesion of Plies should be min. Pass Standard | Excellent | |
4. | Static Bending Strength | ||
MOR Along the Grain | Avg. – 40 N / mm2 Ind. – 36 N / mm2 | Avg. 45.21 N / mm2 Ind. 41.35 N / mm2 | |
MOR Across the Grain | Avg. – 20 N / mm2 Ind. – 18 N / mm2 | Avg. 26.16 N / mm2 Ind. 18.24 N / mm2 | |
MOE Along the Grain | Avg. – 5000 N / mm2 Ind. – 4500 N / mm2 | Avg. 5610.15 N/mm2 Ind. 4945.21 N/mm2 | |
MOE Across the Grain | Avg. – 2500 N / mm2 Ind. – 2200 N / mm2 | Avg. 2831.41 N/mm2 Ind. 2523.17 N/mm2 | |
5. | MyCological Test | Min. Pass Standard | Pass Standard |
6. | Workmanship And Finish | Should be Conforming to The Requirements of Cl. 9.1 & 9.2 of IS – 303 : 1989 | Conforming |